Hostname: page-component-78c5997874-fbnjt Total loading time: 0 Render date: 2024-11-02T22:21:25.608Z Has data issue: false hasContentIssue false

Microstructure of GaN Grown on (111) Si by MOCVD

Published online by Cambridge University Press:  13 June 2014

D. M. Follstaedt
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056
J. Han
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056
P. Provencio
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056
J. G. Fleming
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056

Abstract

Gallium nitride was grown on (111) Si by MOCVD by depositing an AlN buffer at 1080°C followed by GaN at 1060°C. The 2.2 μm layer cracked along {1-100} planes upon cooling to room temperature, but remained adherent. We were nonetheless able to examine the material between cracks with TEM. The character and arrangement of dislocations are much like those of GaN grown on Al2O3: ∼2/3 pure edge and ∼1/3 mixed (edge + screw), arranged in boundaries around domains of GaN that are slightly misoriented with respect to neighboring material. The 30 nm AlN buffer is continuous, indicating that AlN wets the Si, in contrast to GaN on Al2O3.

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society

Introduction

Hexagonal GaN is being widely studied because of its large, direct bandgap and high thermal stability. Applications are envisioned in technologies involving short wavelength (green, blue and UV) optoelectronics and high-temperature or high-power electronics. A key issue for growth of GaN has been the lack of an ideal substrate, since GaN substrates are not readily available and other semiconductors have large lattice mismatches. Most GaN has been grown on sapphire (Al2O3); vapor-phase growth usually begins with deposition of a low temperature GaN buffer followed by the complete layer at near 1000°C. Applications with sapphire are limited by its lack of electrical conductivity and high cost.

We have investigated growth of GaN on Si with the intent of integrating short-wavelength devices into Si-based microelectronics, as well as providing an alternative substrate. We have grown GaN by metal-organic chemical vapor deposition (MOCVD) on (111) Si and obtained microstructures much like those for sapphire, but cracking during cooling to room temperature limits use of our current materials. Here we use transmission electron microscopy (TEM) to examine dislocations in the GaN and the structure of the AlN buffer layer grown at the interface with the Si, and compare them to corresponding microstructures of GaN grown on Al2O3. An introduction to this work and our related approaches to growth on Si is given elsewhere [Reference Han, Flemming and Follstaedt1].

Growth of GaN

A 1000 rpm rotating disk reactor with 4.75″ quartz chamber was used to grow AlN and GaN with trimethylgallium, trimethylaluminum, and ammonia precursors at 30 Torr [Reference Han, Flemming and Follstaedt1]. Several investigations indicate that growing an AlN buffer first on Si avoids the formation of amorphous Si3N4 since N reacts more exothermically with Al than Si; this is important for attaining good epitaxial growth of GaN [Reference Watanabe, Takuchi, Hirosawa, Amano, Hiramatsu and Akasaki2,Reference Guha and Bojarczuk3]. Our methods follow those of Watanabe et al [Reference Watanabe, Takuchi, Hirosawa, Amano, Hiramatsu and Akasaki2] who found that AlN buffer growth at >1000°C leads to good epitaxy, in spite of the 17% lattice mismatch of GaN with Si. We grew a 30 nm AlN buffer at 1080°C, followed by 2.2 μm of GaN at 1060°C.

In situ reflectivity indicated that the GaN surface was smooth immediately after growth at 1060°C. However, upon cooling to room temperature, a dense set of cracks with separations From 20 to 100 μm was found along {1-100} planes, as seen in Figure 1. The layer is expected to have relaxed fully at the growth temperature, as found for GaN grown on Al2O3 using in situ stress monitoring techniques [4]. The greater thermal expansion coefficient of GaN as compared to that of Si (5.6x10-6/K vs.2.6x10-6/K, respectively) then explains cracking since the GaN layer would be put into tension upon cooling. In spite of cracking, the GaN layer adhered to the substrate. X-ray diffraction of such layers gives (0002) GaN reflections with FWHM of 900 arcsec, similar to those found previously [Reference Watanabe, Takuchi, Hirosawa, Amano, Hiramatsu and Akasaki2].

Figure 1. Nomarski optical micrograph showing cracking of GaN on (111) Si along {1-100} planes.

Tem Characterization of Defects in GaN

Cross-section TEM specimens were successfully prepared by usual metallographic polishing and ion milling methods for both [110] and [Reference Han, Flemming and Follstaedt1-12] Si orientations in spite of the cracking. Cracks were found passing directly across the layer and into the Si substrate. The cracks were open with no indication of subsequent deposition, consistent with their forming after growth [Reference Han, Flemming and Follstaedt1]. No evidence of de-adhesion of the layer from the substrate was seen where the cracks cross the interface into the Si. The GaN layer was found to be single phase and with no 30°-misoriented grains as seen in other material grown by molecular beam epitaxy (MBE) [Reference Basu, Lei and Moustakas5]. Selected-area diffraction demonstrated the epitaxial orientation seen previously for GaN on (111) Si [Reference Watanabe, Takuchi, Hirosawa, Amano, Hiramatsu and Akasaki2,Reference Guha and Bojarczuk3,Reference Basu, Lei and Moustakas5]:

Dislocations thread from the buffer layer to the surface of the GaN layer along the c-axis, growth direction. Examination in cross-section with different diffracting beams can be used to determine the Burger’s vectors of individual dislocations, which for hexagonal close-packed lattices are [Reference Hirth and Lothe6]: a (or 1/3<11-20>, in the basal lattice plane), c (<0001>, along the hexagonal axis), or a+c (1/3<11-23>, mixed character). In Figure 2, image (a) uses the (0004) reflection to illuminate the cores of dislocations with Burger’s vectors having a c-axis component. Image (b) uses (1-100) to image those with a basal plane component. Detailed examinations with several reflections indicate that almost all dislocations are detected in Figure 2b) and have a basal-plane component. Those with a c-axis component seen in Fig. 2a (∼1/3 of the total) are almost all of mixed character. The additional ones in Fig. 2b (∼2/3 of the total) have purely basal-plane Burger’s vectors, b = a; since the dislocation lines are fairly straight along the c-axis, these are edge dislocations. Very few dislocations have b = c corresponding to pure screw character. This distribution of Burger’s vectors is like that found by us [Reference Ng, Han, Biefeld and Weckwerth7] and others [Reference Wu, Brown, Kapolnek, Keller, Keller, DenBaars and Speck8] in GaN on sapphire.

Figure 2. Weak-beam TEM images obtained near [Reference Wu, Fini, Keller, Tarsa, Heying, Mishra, DenBaars and Speck11-20] orientation. a) g = (0004), with cores of dislocations having b = a + c illuminated. b) g = (1-100), with cores of all dislocations illuminated. A crack running through the layer and into the Si substrate is seen at far right.

Plan-view TEM gives additional insight into the dislocation arrangement. A specimen was prepared by placing thinned epoxy on the specimen surface to penetrate into cracks, removing excess epoxy from the surface, and carefully backthinning with the specimen attached to a grid for structural support. The thinned area is at the surface of the GaN layer and allows defects threading to it to be detected. In Figure 3, the dislocations are viewed nearly end-on and appear as short black-white segments. They often lie along continuous curves that form boundaries between domains of material with slightly differing orientations. A similar arrangement is found for threading dislocations in GaN grown on sapphire [Reference Ning, Chien, Pirouz, Yang and Khan9]. Plan-view images allow more surface area to be examined than in cross-section and give the most accurate determination of dislocation density at the surface: 8×109 disl/cm2 for this specimen. This density is like that found for GaN grown on sapphire [Reference Ng, Han, Biefeld and Weckwerth7], although lower values have been achieved [Reference Wu, Brown, Kapolnek, Keller, Keller, DenBaars and Speck8].

Figure 3. Plan-view TEM image of the surface of the GaN layer, obtained near [0001] orientation using g = (1-100) two-beam conditions in bright-field. Dislocations appear as short black-white lines, and often form continuous curves at boundaries between domains of material with slightly differing orientations; two are noted with nearby dashed lines. Two void-like defects (nanotubes or pinholes) are also noted with arrows.

By examining this greater surface area, an additional defect with a low density is found. Two void-like defects were identified in Figure 3 (small white spots, arrowed) by examining their contrast with changes in TEM objective lens focus. Such defects have been termed “nanotubes” if they have extended length into the GaN, or “pinholes” if they are pits located at surface [Reference Liliental-Weber, Chen, Ruvimov and Washburn10]. Since we do not have depth information, we cannot determine which of the two classifications apply. Other images taken under high resolution conditions show that the {1-100} lattice planes form facets around the voids. Their areal density is ∼1×108/cm2, again comparable to that found in GaN grown on sapphire [Reference Liliental-Weber, Chen, Ruvimov and Washburn10].

Examination of Aln Buffer Layers

The buffer layer was found to be continuous over extended distances in cross-section images. It’s thickness varies somewhat as seen in Figure 4a, but it is readily identified from the GaN overlayer. By tilting the specimen slightly to vary the contrast in bright field, or by weakbeam examinations like Figure 4b, the layer is seen to be composed of grains that are 20-40 nm across and slightly misoriented with respect to each other.

Figure 4. a) Bright-field, (3-300) two-beam image of AlN buffer on Si near [Reference Wu, Fini, Keller, Tarsa, Heying, Mishra, DenBaars and Speck11-20] cross-section orientation with dislocations extending into GaN layer. b) Corresponding weak-beam image showing 20-40 nm grains in the buffer with contrast between them indicating slight orientation differences. Two dislocations appear to originate at grain boundaries in the buffer (arrowed).

Dislocations in the GaN just above the buffer interact with each other, as seen in Figure 4. The dislocations extend into the AlN buffer at near-normal incidence. In some cases, they appear to coincide with grain boundaries in the buffer; two instances are arrowed in Figure 4b. This suggests that the misorientations between AlN buffer grains may directly produce some of the dislocations threading through the GaN. Perhaps if a buffer layer with larger grains were formed, the GaN would have fewer defects.

Having a continuous 30 nm-thick AlN layer on Si implies that the AlN “wets” the Si under our conditions, indicating that the AlN/Si interface has lower energy than the AlN/vacuum surface. A continuous AlN layer was also found for an even thinner (8 nm) buffer grown on Si by MBE [Reference Guha and Bojarczuk3]. Such continuous layers differ greatly from those observed for GaN grown by MOCVD on Al2O3 using a low-temperature buffer layer followed by high-temperature growth. For GaN/Al2O3 the layer must be 0.4 μm thick before it is continuous [Reference Liliental-Weber, Chen, Ruvimov and Washburn10]. The wetting may indicate that more favorable bonding is occuring between nitrides and the Si. Such good bonding is suggested by the adhesion of the layer to the substrate as evidenced by the cracks propagating across the interface instead of along it. Thus Si appears to be the preferred substrate for initiating growth of nitrides when used with an AlN buffer.

A cross-section TEM specimen was also made of a 40 nm-thick AlN buffer layer grown alone on (111) Si at 1100°C. The layer was again found to be continuous with slight misorientations between grains, as seen in Figure 5. Our examinations indicated two other features of this layer. First the individual grains composing the buffer exhibit faceting on the growth surface; the facets appear to be {1-101} lattice planes. Secondly, a few voids were found in the Si immediately beneath the interface, which suggests that Si may be diffusing into the AlN.

Figure 5. Cross-section TEM image of 40 nm AlN buffer grown on (111) Si, seen in [Reference Wu, Fini, Keller, Tarsa, Heying, Mishra, DenBaars and Speck11-20] orientation with g = (0002) two-beam conditions. Grains in the AlN buffer are faceted at the top surface, and two voids (arrowed) can be seen just below the interface in the Si.

Discussion

Microstructural features of GaN grown on Si are compared with those for growth on sapphire in Table I. Cracking clearly remains a problem for the Si substrate that must be overcome before devices can be made. The microstructures of threading dislocations are very similar in GaN grown on the two substrates; in both cases the threading dislocations appear due to small local misorientations between adjacent materials. It may be possible to influence the dislocation density with Si by varying the growth conditions of the AlN buffer.

Table I. Comparison of Microstructures: GaN/Al2O3 versus GaN/Si

GaN/Al 2 O 3 GaN/Si (this work)
Cracking: no yes, {1-100} planes
Dislocations: density 108 – 1010 /cm2 [Reference Ng, Han, Biefeld and Weckwerth7-Reference Ning, Chien, Pirouz, Yang and Khan9] 8x109 /cm2
character 1/3 mixed, 2/3 edge [Reference Wu, Brown, Kapolnek, Keller, Keller, DenBaars and Speck8] 1/3 mixed, 2/3 edge
arrangement boundaries [Reference Ning, Chien, Pirouz, Yang and Khan9] domain walls
nanotubes, pinholes 106 – 108 /cm2 [Reference Liliental-Weber, Chen, Ruvimov and Washburn10] ∼108 /cm2
Buffer: type (temperature) GaN (550°C) [Reference Ng, Han, Biefeld and Weckwerth7] AlN (1080°C)
wetting no yes
thickness for continuity ∼0.4 μm [Reference Wu, Fini, Keller, Tarsa, Heying, Mishra, DenBaars and Speck11] ∼ 30 nm
microstructure faulted (hcp/fcc) [Reference Wu, Brown, Kapolnek, Keller, Keller, DenBaars and Speck8] hcp grains (20-40 nm)

The buffer layers are very different, with AlN wetting Si but GaN not wetting Al2O3 even after subsequent high-temperature growth. This difference this may reflect a change in bonding across the interface, although differing deposition temperatures and differences between AlN and GaN need to be considered. Since Si is covalent whereas Al2O3 is ionic, the change may be due to covalent bonding of the AlN to the Si. The faulting seen [Reference Wu, Brown, Kapolnek, Keller, Keller, DenBaars and Speck8] in nucleation layers for GaN on Al2O3 is associated with the low-temperatures needed to induce growth of GaN, which then occurs in both its fcc and hcp phases; we have not detected faulting in our high-temperature AlN buffer layers.

Acknowledgments

The authors would like to thank S. Hearne and J. Floro for discussions about stress in GaN layers during growth, and S. R. Lee for discussions about cracking in GaN layers on Si. This work at Sandia National Laboratories supported by the United States Department of Energy under Contract DE-AC04-94Al85000. Sandia is a multiprogram laboratory operated by Sandia Corporation, a Lockheed Martin Company for the United States Department of Energy.

Footnotes

MRS Internet J. Nitride Semicond. Res. 4S1, G3.72 (1999)

References

Han, J., Flemming, J. G. and Follstaedt, D. M., Mat. Res. Soc. Symp. Proc. 512, 53 (1998).CrossRefGoogle Scholar
Watanabe, A., Takuchi, T., Hirosawa, K., Amano, H., Hiramatsu, K. and Akasaki, I., J. Crystal Growth, 128, 391-396 (1993).CrossRefGoogle Scholar
Guha, S. and Bojarczuk, N. A., Appl. Phys. Lett. 72, 415 (1998).CrossRefGoogle Scholar
Hearne, S., Floro, J. A. and Tsong, I., private communication (in situ stress measurements).Google Scholar
Basu, S. N., Lei, T. and Moustakas, T. D., J. Mater. Res. 9, 2370 (1994).CrossRefGoogle Scholar
Hirth, J. P. and Lothe, J., Theory of Dislocations, 2nd ed. (Krieger Publishing Co., Malabar, FL, 1992) p. 270.Google Scholar
Dislocations were analyzed as described herein; the growth of our GaN on sapphire is discussed by Ng, T.-B., Han, J., Biefeld, R. M. and Weckwerth, M. V., J. Electron. Mat. 27, 190 (1998).CrossRefGoogle Scholar
Wu, X. H., Brown, L. M., Kapolnek, D., Keller, S., Keller, B., DenBaars, S. P. and Speck, J. S., J. Appl. Phys. 80, 3228 (1996).CrossRefGoogle Scholar
Ning, X. J., Chien, F. R., Pirouz, P., Yang, J. W. and Khan, M. A., J. Mater. Res. 11, 580 (1996).CrossRefGoogle Scholar
Liliental-Weber, Z., Chen, Y., Ruvimov, S. and Washburn, J., Phys. Rev. Lett. 79, 2835 (1997).CrossRefGoogle Scholar
Wu, X.H., Fini, P., Keller, S., Tarsa, E.J., Heying, B., Mishra, U.K, DenBaars, S.P. and Speck, J.S., Jpn. J. Appl. Phys. Pt.2, 35 L1648 (1996).CrossRefGoogle Scholar
Figure 0

Figure 1. Nomarski optical micrograph showing cracking of GaN on (111) Si along {1-100} planes.

Figure 1

Figure 2. Weak-beam TEM images obtained near [11-20] orientation. a) g = (0004), with cores of dislocations having b = a + c illuminated. b) g = (1-100), with cores of all dislocations illuminated. A crack running through the layer and into the Si substrate is seen at far right.

Figure 2

Figure 3. Plan-view TEM image of the surface of the GaN layer, obtained near [0001] orientation using g = (1-100) two-beam conditions in bright-field. Dislocations appear as short black-white lines, and often form continuous curves at boundaries between domains of material with slightly differing orientations; two are noted with nearby dashed lines. Two void-like defects (nanotubes or pinholes) are also noted with arrows.

Figure 3

Figure 4. a) Bright-field, (3-300) two-beam image of AlN buffer on Si near [11-20] cross-section orientation with dislocations extending into GaN layer. b) Corresponding weak-beam image showing 20-40 nm grains in the buffer with contrast between them indicating slight orientation differences. Two dislocations appear to originate at grain boundaries in the buffer (arrowed).

Figure 4

Figure 5. Cross-section TEM image of 40 nm AlN buffer grown on (111) Si, seen in [11-20] orientation with g = (0002) two-beam conditions. Grains in the AlN buffer are faceted at the top surface, and two voids (arrowed) can be seen just below the interface in the Si.

Figure 5

Table I. Comparison of Microstructures: GaN/Al2O3 versus GaN/Si