Hostname: page-component-586b7cd67f-2brh9 Total loading time: 0 Render date: 2024-11-27T05:48:56.288Z Has data issue: false hasContentIssue false

Ion Channeling Analysis of Gallium Nitride Implanted with Deuterium

Published online by Cambridge University Press:  13 June 2014

W. R. Wampler
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056, [email protected]
S. M. Myers
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-1056, [email protected]

Abstract

Ion channeling and transmission electron microscopy were used to examine the microstructure of GaN implanted with deuterium (D) at high (>1 at. %) and low (< 0.1 at. %) D concentrations. At high concentrations, bubbles and basal-plane stacking faults were observed. Ion channeling showed the D was disordered relative to the GaN lattice, consistent with precipitation of D2 into bubbles. At low D concentrations, bubbles and stacking faults are absent and ion channeling shows that a large fraction of the D occupies sites near the center of the c-axis channel.

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society

Introduction

Hydrogen is incorporated into GaN during growth by MOCVD and also during subsequent processing [Reference Pearton and Pearton1]. This hydrogen strongly affects the electrical properties by passivation of dopants and lattice defects. Release of hydrogen from GaN films requires annealing at temperatures above 800°C [Reference Zavada, Wilson, Abernathy and Pearton2]. However, large reductions in resistivity of Mg doped GaN can be achieved by annealing at lower temperatures where H is not released from the material [Reference Miyachi, Tanaka, Kimura and Ota3,Reference Pearton, Lee and Yuan4]. This indicates that the atomic configuration of H within the GaN lattice significantly affects its influence on electrical properties.

Here we use ion channeling to examine the lattice location of deuterium implanted into wurtzite GaN. Results from the channeling measurements are compared with first-principles calculations of the lattice configuration of hydrogen in GaN [Reference Neugebauer and Van de Walle5,Reference Van de Walle6]. In addition, we use ion channeling and TEM to examine lattice defects produced by the implantation of deuterium.

Experimental Procedures

Wurtzite GaN films with (0001) orientation and thickness in the range of 1.4 - 2.3 µm were grown epitaxially by MOCVD on 420 µm thick c-oriented sapphire substrates as described elsewhere [Reference Han, Ng, Biefeld, Crawford and Follstaedt7]. The GaN was n-type with a carrier density of ∼ 1017/cm3 as determined by conductivity and Hall-effect measurements. The samples were implanted at room temperature with deuterium (D) at 50 keV to fluences of 1015/cm2 and 1017/cm2. This gives D concentration profiles peaking 0.4 μm beneath the surface at concentrations of about 0.05 and 5 atomic % for these two fluences [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8].

Ion channeling measurements were done with the samples mounted on a 3 axis goniometer. D was analyzed by counting protons from the D(3He,p)α nuclear reaction with an incident beam of 0.85 MeV 3He+ ions. With this energy D at depths up to about 1 µm will be detected and the peak in the nuclear reaction cross section [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8] at 0.6 MeV occurs at the depth of the D. Analysis beams of 2 MeV 4He were used to examine lattice damage caused by the D implantation. Energy spectra of 4He backscattered at 155 degrees were recorded for angles of incidence near the c-axis. The analysis beam size was typically 1 mm square and the angular divergence was 0.05 degree.

Experimental Results and Interpretation

Lattice defects due to D implantation

Transmission electron microscopy, both plan view and cross section, shows that GaN implanted with 50 keV H to fluences of 2×1016/cm2 and 1017/cm2 and then vacuum annealed at 886°C for one hour, contains cavities with a typical size of 10 nm at the H implant depth [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8]. These cavities are believed to result from precipitation of H2 gas. Such samples also contain planar defects typically ∼50 nm in diameter, which are shown by high resolution imaging [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8] to be (0001) basal plane stacking faults containing one extra Ga-N bilayer bounded by a partial edge dislocation loop with a Burgers vector c/2[0001]. The atomic configuration of such faults has been discussed elsewhere [Reference Liliental-Weber, Kisielowski, Ruvimov, Chen, Washburn, Grzegory, Bockowski, Jun and Porowski9]. TEM showed these cavities and stacking faults were not present in GaN implanted with H to a lower fluence of 1015/cm2 and annealed at 886°C. The cavities and stacking faults can be seen in the micrographs shown in figure 1.

Fig. 1. Cross-section TEM of a bubble (a) and a stacking fault (b) in GaN implanted with 2×1016 H/cm2 and then vacuum annealed at 886°C for one hour. The bars indicate 5 nm.

Figure 2 shows channeled backscattering spectra for 2 MeV 4He incident along the [0001] axis for GaN implanted at room temperature with 1017 D/cm2. Also shown for comparison is a spectrum for an off-axis unchanneled or random direction obtained by averaging spectra taken at several off-axis orientations, and a channeled spectrum taken on a sample as-grown, i.e. not implanted with D. The channeled spectrum for a low-dose (1015/cm2) implanted sample (not shown) was the same as those for unimplanted samples. The low backscattering yield for axial channeling in the unimplanted GaN of ∼ 2% of random yield near the surface and 3.2% of random yield at the depth of D implantation, is consistent with a film which has few lattice defects.

Fig. 2. Energy spectra for channeled 2 MeV 4He backscattered from GaN. Yield from the implanted region appears at channels in the range from 90-120, while the surface corresponds approximately to channel 140.

Room-temperature implantation of 1017 D/cm2 at 50 keV creates a direct scattering peak, which is shaded in the figure, at an energy corresponding to He scattered from Ga at the depth of the implanted D, and increases the yield at lower energies due to dechanneling. Subsequent one hour vacuum anneals in the temperature range 511-709°C removes the direct scattering peak and increases the dechanneling step. The direct scattering peak shows that prior to annealing, Ga atoms are displaced from lattice sites into the open [0001] channel, thereby enhancing the backscattering yield of channeled 4He ions. We refer to these displaced Ga atoms generically as Ga interstitials without implying a specific lattice location. The disappearance of this direct scattering peak with annealing indicates a return to lattice sites. The associated increase in dechanneling is consistent with the formation of extended defects with large strain fields, eg. dislocations, which dechannel the 4He with little direct scattering. Reference 10 gives more detailed discussion of defect analysis by ion channeling.

The area under the direct scattering peak can be used to calculate the areal density of Ga interstitials. The number of counts in the peak is given by

(1)

where NHe is the number of incident 4He ions, σR is the Rutherford differential cross section for scattering of 4He from Ga, Ω is the solid angle subtended by the detector, Ni is the areal density of interstitial Ga and f is the flux enhancement due to channeling at the location of the interstitial Ga. With Y = 3500 from the channeled spectrum before annealing (fig. 2) and f = 2 from computer simulations (discussed later) of 4He channeling in GaN assuming all Ga interstitials are near the center of the [0001] channel, we obtain Ni = 3.0×1016/cm2. This number is smaller by two orders of magnitude than the areal density of collisional displacements caused by the D implantation, which is estimated to be ∼40 displacements per incident ion or 4×1018 displacements/cm2. However, the areal density of Ga interstitials estimated from the direct scattering peak is close to the areal density 3.5 × 1016/cm2 of Ga atoms displaced by the bubbles [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8]. This result suggests the following model for bubble formation: the vacancies and interstitials produced by atomic displacements mostly recombine, however a small fraction of the vacancies agglomerate and combine with H to form high pressure H2 bubbles, leaving a corresponding number of interstitials in the neighboring lattice. At temperatures in the range from 500 to 700°C most of these interstitials annihilate, possibly by diffusing to the surface while some agglomerate into the stacking faults seen by TEM.

If it is assumed that the dechanneling step is due to strain fields from the dislocation loops bounding the stacking faults, then the number of these defects and the areal density of interstitial atoms enveloped by them can be estimated from the height of the dechanneling step. In general the areal density of a defect is related to dechanneling by the equation [Reference Feldman, Mayer and Picraux10]

(2)

were χD is the channeled backscattering yield above the step divided by the random or unchanneled yield, and χv is the corresponding quantity in the absence of defects. The cross section for dechanneling by the strain field of a dislocation is given by [Reference Feldman, Mayer and Picraux10]

(3)

where aTF is the Thomas-Fermi screening distance, b is the length of the Burgers vector, ψ1 is a critical angle for dechanneling. Using a value K=1.2, derived elsewhere for axial channeling perpendicular to an edge dislocation [Reference Quéré11], we obtain σd = 5.3×10−7 cm2/cm. With χv = 0.032 and χD = 0.19 from the channeled spectrum after annealing at 809°C, eq. 2 yields ND = 3.4×10−5 cm/cm2. Assuming the stacking faults are circular with a diameter of 50 nm estimated from TEM, this value of ND implies that the associated areal density of extra Ga and N atoms is 1.0×1015/cm2. This number is smaller by a factor of 70 than the areal density of Ga and N atoms calculated to be displaced by bubble formation.

We also conclude that the bubbles themselves do not contribute significantly to direct scattering and dechanneling. The combined basal plane area of the bubbles per unit sample area is estimated to be ∼3 cm2/cm2 [Reference Myers, Headley, Hills, Han, Petersen, Seager and Wampler8]. If the He ions re-enter the lattice at random locations after traversing a bubble, the direct scattering and dechanneling from the bubbles should be about three times that of the external surface, which is small compared to the observed direct scattering and dechanneling as can be seen in figure 2.

Location of D in the GaN lattice

The location of foreign atoms relative to the host lattice can be determined by ion channeling [Reference Feldman, Mayer and Picraux10]. Here we use the D(3He,p)α nuclear reaction to study the lattice location of D implanted into GaN. The yield is proportional to the local flux of 3He at the location of the D. For angles of incidence far from major axes or planes the flux of 3He is nearly the same at all locations in the lattice. However, when the analysis beam is aligned along the c-axis, channeling reduces the flux near the rows of host atoms and increases the flux near the center of the open channels relative to fluxes with off-axis alignment. This will give rise to a dip in the NRA yield if the D is near the host atom rows, for example at a substitutional site, or conversely, to a peak in the NRA yield if the D is near the center of the channel. The absence of a peak or dip would indicate that the D is randomly located relative to the lattice.

Figure 3 shows the measured NRA yield normalized to the off-axis or random yield versus the angle between the analysis beam direction and the c-axis. For GaN implanted to the low dose of 1015 D/cm2 there is a narrow peak ∼40% above the random yield, whereas for GaN implanted with 1017 D/cm2 there is no peak. The absence of a peak for the high dose implanted sample is consistent with the idea that at high concentrations most of the D precipitates as gas into cavities which would give random location for the D relative to the GaN lattice sites. The peak for the low dose sample shows that a large fraction of the D is in the open channels. The height of this peak was observed to be a function of the analysis beam dose. Figure 4 shows the peak height as a function of off-axis 3He analysis beam dose to the sample. The increase in peak height with beam dose shows that the analysis beam is causing the D to change its location in the lattice. The increase saturates after a few microcoulombs. The data shown in figure 3 were all taken after this beam induced increase had saturated. Measurements of the NRA yield after one hour vacuum anneals showed the peak remained unchanged up to 411°C, decreased with increasing temperature above 511°C, and became poorly resolved by 809°C.

Fig. 3. NRA yield versus angle from the c axis.

Fig. 4. NRA yield at axial alignment verses off-axis beam dose for GaN implanted with 1015D/cm2.

We have carried out computer simulations of the yield versus angle for various D locations in the GaN lattice. These simulations were done using a statistical equilibrium continuum (SEC) model [Reference Bech-Nielsen12] modified for the case of channeling along the c-axis in wurtzite GaN. The SEC model has previously been used to determine the lattice location of D implanted into silicon [Reference Bech-Nielsen12]. Our calculations use Doyle Turner potentials [Reference Doyle and Turner13] for the GaN lattice with 24 rows. The model includes dechanneling due to thermal vibration of the host atoms. RMS vibrational amplitudes of 0.00735 nm for Ga and 0.00806 nm for N were used [Reference Yoshiasa, Koto, Maeda and Ishii14]. The SEC model gave good agreement with the observed channeling dip for 2 MeV 4He backscattered from the host lattice as shown in figure 5, providing an important validation of the model. The NRA yield curves were calculated using a vibrational amplitude of 0.010 nm for the D. The D vibrational amplitude was estimated assuming a harmonic oscillator model with a vibrational frequency of ∼ 2300 cm−1 for the D-N stretch mode determined from infrared absorption measurements [Reference Weinstein, Song, Stavola, Pearton, Wilson, Shul, Killeen and Ludowise15] and from first principles calculations [Reference Liliental-Weber, Kisielowski, Ruvimov, Chen, Washburn, Grzegory, Bockowski, Jun and Porowski9]. Except for the S site, changes in D vibrational amplitude by factors of 2 do not significantly change the calculated yield curves. The yields calculated by the SEC model correspond to values averaged over all azimuthal angles. In order to compare with the SEC model, the data shown in figures 3 (NRA) and 4 (RBS) are averages of measurements at many azimuthal angles.

Fig. 5. Solid curves show the NRA yield versus angle calculated by the SEC model for D at the various indicated locations in the c-axis channel. The calculated backscattered yield (dashed curve) agrees well with measured azimuthally averaged yield (dots) of backscattered 2 MeV 4He

Figure 5 shows the yield predicted by the SEC model for various locations of D in the channel as indicated in the inset diagram. Curve C is for D at the channel center, curve S is for D in line with the host atom rows which includes substitutional sites. Also shown is the yield for D at a bond-center site midway between the Ga and N atoms at the channel edge. Another site which has been proposed for hydrogen in GaN is the nitrogen antibonding site which is along the tetrahedral bond direction ∼0.10 nm from the N atoms but opposite the neighboring Ga atoms [Reference Van de Walle6]. The channeling yield curves for the one quarter of nitrogen antibonding and bond center sites in-line with the host atom rows, are the same as for the S site. The yield curves for the remaining three quarters of these sites, at locations indicated in the inset diagram as BC and AB in the inset diagram, are shown in figure 5. In the wurtzite structure the two types of AB and BC sites are not equivalent and need not be equally occupied by D. The peak we observe in the measured NRA yield shows that a large fraction, of order 50% or more, of the D occupies sites near the channel center such as the C or AB sites in the sample implanted with 1015 D/cm2.

The increase in NRA channeling yield with analysis beam dose which we observe, and the fact the D depth distribution does not broaden during thermal release, suggest that the D is bound at lattice defects. First-principles calculations have been reported for H bound to vacancies in GaN [Reference Van de Walle6]. These calculations predict that H in a N vacancy will be located near the center of the vacancy. Accordingly, D trapped at N vacancies is expected to be located substitutionally at the N lattice site which would correspond to the S site shown in figure 5. Our NRA channeling data excludes significant occupation of D at this site.

D in a Ga vacancy should form a strong covalent bond with one of the N neighbors [Reference Van de Walle6]. This would place the D about 0.10 nm from an N atom along the tetrahedral bond direction. Since the GaN bond length is 0.20 nm the predicted position for D in a Ga vacancy is therefore very close to the bond center location, in the absence of relaxation of the lattice around the vacancy. Therefore, the yield curves for D in a Ga vacancy for the N whose bond is along the c direction, should be similar to the curve for the S site. For D bound to the other three N, the yield curve should be similar to that of the BC site shown in figure 5. Both of these sites for D at a Ga vacancy give a dip in the channeling yield as shown in figure 5. In a recent study, IR absorption bands were observed due to H-N and D-N stretch mode vibrations in GaN implanted with H and D [Reference Weinstein, Song, Stavola, Pearton, Wilson, Shul, Killeen and Ludowise15]. These absorption bands were tentatively assigned to H or D bound to N at Ga vacancies. Our channeling results show that most of the implanted D is not at such sites since this would give a dip in the NRA channeling yield in contrast to the peak we observe. It therefore seems appropriate to consider other defect-related sites, including interstitials or solution sites adjacent to defects as possible binding sites for D.

Acknowledgments

The authors thank Jung Han for supplying the GaN and Alan Wright for insightful discussions of energy and structure calculations for hydrogen in GaN. This work was supported by the U.S. Department of Energy under contract DE-AC04-94AL8500, in part under auspices of the Office of Basic Energy Sciences. Sandia National Laboratories is a multi-program laboratory operated by Sandia Corporation, a Lockheed Martin Company, for the U.S. Department of Energy.

Footnotes

MRS Internet J. Nitride Semicond. Res., 4S1, G3.73 (1999)

References

Pearton, S. J., in GaN and related materials, edited by Pearton, S. J. (Gordon and Breach, London, 1997) chapter 14.Google Scholar
Zavada, J. M., Wilson, R. G., Abernathy, C. R. and Pearton, S. J., Appl. Phys Lett. 64, 2724 (1994).Google Scholar
Miyachi, M., Tanaka, T., Kimura, Y., Ota, H., Appl. Phys. Lett. 72, 1101 (1998).Google Scholar
Pearton, S. J., Lee, J. W., and Yuan, C., Appl. Phys. Lett. 68, 2690 (1996).Google Scholar
Neugebauer, J., and Van de Walle, C. G., Phys. Rev. Lett. 75, 4452 (1995).Google Scholar
Van de Walle, C. G., Phys. Rev. B56, 10020 (1997).Google Scholar
Han, J., Ng, T. B., Biefeld, R. M., Crawford, M. H., and Follstaedt, D. M.. Appl. Phys Lett. 71, 3114 (1997).CrossRefGoogle Scholar
Myers, S. M., Headley, T. J., Hills, C. R., Han, J., Petersen, G. A., Seager, C. H. and Wampler, W. R., MRS Internet J. Nitride Semicond. Res. 4S1,G5.8 (1999).Google Scholar
Liliental-Weber, Z., Kisielowski, C., Ruvimov, S., Chen, Y., Washburn, J., Grzegory, I, Bockowski, M., Jun, J. and Porowski, S., J. Electron. Mater. 25, 1545 (1996).Google Scholar
Feldman, L. C., Mayer, J. W. and Picraux, S. T., Materials Analysis by Ion Channeling, (Academic, New York, 1982), pp. 88-135.Google Scholar
Quéré, Y., Phys. Stat. Sol. 30, 713 (1968).Google Scholar
Bech-Nielsen, B., Phys. Rev. B37, 6353 (1988).Google Scholar
Doyle, P. A. and Turner, P. S., Acta Crystalogr. Sect.A 24, 390 (1968).Google Scholar
Yoshiasa, A., Koto, K., Maeda, H. and Ishii, T., Jpn. J. Appl. Phys. 36, 781 (1997).Google Scholar
Weinstein, M. G., Song, C. Y., Stavola, M., Pearton, S. J., Wilson, R. G., Shul, R. J., Killeen, K. P. and Ludowise, M. J., Appl. Phys Lett. 72, 1703 (1998).Google Scholar
Figure 0

Fig. 1. Cross-section TEM of a bubble (a) and a stacking fault (b) in GaN implanted with 2×1016 H/cm2 and then vacuum annealed at 886°C for one hour. The bars indicate 5 nm.

Figure 1

Fig. 2. Energy spectra for channeled 2 MeV 4He backscattered from GaN. Yield from the implanted region appears at channels in the range from 90-120, while the surface corresponds approximately to channel 140.

Figure 2

Fig. 3. NRA yield versus angle from the c axis.

Figure 3

Fig. 4. NRA yield at axial alignment verses off-axis beam dose for GaN implanted with 1015D/cm2.

Figure 4

Fig. 5. Solid curves show the NRA yield versus angle calculated by the SEC model for D at the various indicated locations in the c-axis channel. The calculated backscattered yield (dashed curve) agrees well with measured azimuthally averaged yield (dots) of backscattered 2 MeV 4He