Previous studies addressing the segregation of reactive elements in protective oxide scales and their beneficial effect on scale adhesion have primarily concentrated on primary alumina-formers (e.g. β-NiAl + FeCrAl).In our study the oxidation behaviour of three NiCrAl alloys, which form complex scales was studied in air at 1423 K and at 1473 K, both in isothermal (100 h) and in cyclic oxidation (100 x lh). The composition (in at.-%) of these alloys is the following: General Electric alloy René N5 (64.9 Ni, 7.8 Cr, 13.9 Al, 0.1 Fe, 2.1 Ta, 0.05 Hf, 1.6 W, 1.0 Re, 0.15 Si, 7.3 Co, 0.9 Mo, 0.003 Y, 0.003 Zr, 4 ppm S, 0.25 C), Ni-7Cr-6.5Al+Y (80.1 Ni, 7.2 Cr, 12.5 Al, 0.01 Fe, 0.14 Si, 0.012 Y, 18 ppm S, 0.05 C) and Ni-10Cr-10Al+Y (71.2 Ni, 9.9 Cr, 18.8 Al, 0.01 Fe, 0.02 Si, 0.041 Y, 16 ppm S, 0.04 C).