Hostname: page-component-78c5997874-fbnjt Total loading time: 0 Render date: 2024-11-06T22:20:27.079Z Has data issue: false hasContentIssue false

Growth on GaN and GaAs on fianite by MOCVD capillary epitaxy technique

Published online by Cambridge University Press:  13 June 2014

A. N. Buzynin
Affiliation:
General Physics Institute of RAS
V. V. Osiko
Affiliation:
General Physics Institute of RAS
Yu. N. Buzynin
Affiliation:
Institute for Physics of Microstructure of RAS
B. Pushnyi
Affiliation:
Ioffe Physical-Technical Institute

Abstract

Heteroepitaxial GaN and GaAs films were grown by both conventional two-step MOCVD and the new “capillary epitaxy” technique on (001) and (111) fianite (YSZ) substrates. The capillary epitaxy technique was investigated for the example of GaAs films growth on a YSZ substrate. This technique allows both the reduction of the minimum thickness and the improvement of the quality of III-V films. PL spectra of undoped GaN films on YSZ were studied.

Type
Research Article
Copyright
Copyright © 1998 Materials Research Society

1. Introduction

Fianite (or yttria stabilized zirconia - YSZ) has a number of significant advantages in comparison with other insulating substrate materials, as follows: good insulating properties (1012Om.cm at 300K); and high optical transmission in a wide wavelength range including the visible. Fianite is a good epitaxial partner for AIIIBV compounds because of their crystallochemical and physical characteristics (table 1).

Table I Some characteristics of YSZ and AIIIBV crystals.

Epitaxial Si films on YSZ prepared by the pyrolysis of silane in a hydrogen atmosphere Reference Mercardalli, Diemegand, Crose and Siejka[1] and by the chloride vapor phase technique Reference Manasevit, Goleski and Mondy[2] at a temperature of more than 1000°C have been reported. To diminish the negative role of the difference in thermal expansion coefficients between epitaxial pairs it is necessary to lower the epitaxial temperature to about 650°C. We have reported about thin GaAs films on YSZ prepared by the metallorganic chemical vapor deposition (MOCVD) Reference Buzynin, Buzynin and Osiko[3]. GaAs films on YSZ substrates have better properties than those on either sapphire or SI-GaAs due to better structural and electrical characteristics, and better thermal and radiation stability.

In this paper we report new results about GaN and GaAs films grown on YSZ substrates by the MOVPE and “capillary epitaxy” Reference Busynin, Buzynin and Osiko[4] technique. The source materials were TMG and AsH3 for GaAs or NH3for GaN3 films. The films have been characterized by electron microscopy (TEM and SEM), X-ray diffraction (XRD), reflection high-energy electron diffraction (RHEED), luminescence, secondary - ion mass spectroscopy (SIMS) and Van der Pauw measurements.

2. Experiment

2.1 Preparation of the YSZ Substrates

The single YSZ crystals, consisting of ZrO2 stabilized with 10, 15 and 21 mole per cent of Y2O3, were grown by the skull melting technique Reference Aleksandrov, Osiko, Prokhorov and Tatarintsev[5] at 3000°C in air (RF power – 160 kW, frequency – 1.67 MHz). The YSZ crystal block dimensions were large (40-80 mm in cross section and 80-100 mm in length). As-grown YSZ crystals can have both block crystalline and single crystalline structure. We used only single crystalline YSZ with the best structural perfection for wafer preparation. YSZ (100) and (111) oriented wafers were prepared by a multistage technique Reference Shabunov, Shengurov and Buzynin[6] using ultra dispersed diamond at the mechanical treatment stage.

The chemical composition of the YSZ crystals has been confirmed by x-ray wavelength dispersion analysis using the “Camebax 50SX” SEM. The analysis of impurity compositions of both bulk YSZ crystals and the surface layer of wafers has been performed by x-ray fluorescence spectral analysis using the “VRA-3” instrument. The results of this investigation (Table 2) showed that the mechanical treatment of crystals resulted in the increase of some impurity concentration (Al, Ca, Na, K, Si). The wafers were subjected to additional annealing in order to reduce the concentration of these impurities and to optimize the physical-chemical state of wafer surface before the epitaxy. Recrystallization annealing of YSZ wafers resulted in both removal of impurities and improvement of crystal perfection [7].

Table II Impurity concentration in YSZ single crystals, YSZ-wafers and GaAs/YSZ films

2.2 Capillary epitaxy of GaAs on YSZ

The capillary epitaxy technique Reference Busynin, Buzynin and Osiko[4] is based on covering the YSZ wafer with the thin film of A component, and subsequently saturating the film with the corresponding B component until the formation of III-V continuous layer. After that, III-V films were grown to the needed thickness. This technique was studied for the example of GaAs heteroepitaxial growth on YSZ substrates. It was found that the GaAs layers could be grown only within a narrow temperature range of about 550-600°C. When the buffer Ga layer is absent the films have polycrystalline structure and a rough surface. The minimum thickness of these films was about 1,5-2μ. In contrast, thin (50 nm) GaAs films can be obtained after Ga layer formation using the “capillary epitaxy” technique Reference Busynin, Buzynin and Osiko[4].

Figure 1 shows SEM micrographs of GaAs films prepared on YSZ by both conventional MOCVD (Figure 1a) and the capillary epitaxy technique (Figure 1b) at the initial stage of growth, and NH4J graphoepitaxy on an amorphous Al substrate (Figure 1c,1d). An analogy between the helpful action of capillary forces for the new capillary epitaxy technique and for graphoepitaxy was suggested earlier Reference Sheftal and Buzynin[8]. The formation of layers in both capillary epitaxy and the graphoepitaxy technique take place from creation and coalescence of three-dimensional nuclei. As in the case of graphoepitaxy using surface active substances Reference Sheftal and Buzynin[8], the use of capillary forces at the first heteroepitaxial stage of the GaAs/YSZ film formation resulted in the following consequences:

  1. 1. epitaxial nuclei density increased;

  2. 2. the nucleus dimension decreased;

  3. 3. the nucleus habit became more flat;

  4. 4. the epitaxial orientation of the nuclei improved.

Figure 1 SEM micrographs of GaAs films prepared using both conventional MOCVD (a) and capillary epitaxy MOCVD(b) at the initial stage of epitaxy on YSZ substrates (60 and 600s after procedure beginning, 20000x) and optical micrographs of NH4J flat crystals prepared by the graphoepitaxy technique on amorphous Al substrates without (c) and with(d) a surface active substance (100x).

As a result, the minimum GaAs/YSZ film thickness was decreased to 50 nm, and the structural perfection and surface morphology of the films were improved. Single crystalline 50-500 nm thick GaAs(100) films on YSZ(100) were prepared. The submicron GaAs films grown by the capillary epitaxy technique had high resistance. For n-type GaAs films, SiH4 was used as dopant source. Electron concentration in the films was in the range of 5·1016 to 5·1017cm-3. SIMS data showed that background impurity concentration was similar to that in GaAs/GaAs films. The layer -by-layer SIMS analysis indicated a uniform distribution of impurities in the GaAs films and a sharp distribution of Zr, O and Y across the film-substrate interface.

According to figure 1, better wetting of substrate led to better film structure both for graphoepitaxy of NH4 on amorphous Al and capillary epitaxy of GaAs on YSZ.

2.3 GaN Films on YSZ

GaN films on YSZ substrates were grown both by conventional MOVPE Reference Ramer and Malloy[9] and by the “capillary epitaxy” Reference Aleksandrov, Osiko, Prokhorov and Tatarintsev[5] technique similarly to the GaAs films. The thin (∼50nm) Ga layer on the YSZ substrate was pre-deposited by the MOD technique before the GaN MOVPE growth in TMG-NH3-H2 system at 1025°C in the case of the “capillary epitaxy” technique. The GaN films had a mosaic structure. The film-substrate orientation relationships are GaN(0001)/YSZ(100) and GaN(0001)/YSZ(111). Typical examples of PL spectra of undoped n-GaN films are shown in Figure 2.

Figure 2. Luminescence spectra of undoped GaN films on a YSZ substrate.

The work on improvement of the structural perfection of GaN films on YSZ substrates is in progress.

3. Summary

GaN and GaAs films were grown by conventional MOCVD and by a new capillary epitaxy technique on YSZ substrates We have studied the capillary epitaxy growth of GaAs films on YSZ substrates in detail. There is an analogy between the helpful action of capillary forces in capillary epitaxy technique and graphoepitaxy using surface-active substances. Use of capillary forces allows both the reduction of the minimum thickness and the improvement of III-V film quality. The growth condition for GaAs submicron single crystalline films with high structural perfection have been established. The grown GaN films had mosaic structure. The film-substrate orientation relationships were GaN(0001)-YSZ(001), GaN(0001)-YSZ(111) and GaAs(001)-YSZ(001). The luminescence spectra of undoped n-GaN films on YSZ substrates were obtained.

Acknowledgments

The authors thank Drs. E.E.Lomonova, A.S.Usikov and W.V.Lundin for some technical assistance. This work was supported in part by Russian State Science-Technology Program “Technologies and Devices of Micro- and Nanoelectronics”, project N 02.04.317.89.4.2

References

Mercardalli, L. M., Diemegand, D., Crose, M., Siejka, Y., Proc. SPIE 623, 183 (1986).CrossRefGoogle Scholar
Manasevit, H. M., Goleski, I., Mondy, L. A., J. Electrochem. Soc. 130, 1752 (1983).CrossRefGoogle Scholar
Buzynin, A.N., Buzynin, Yu.N., Osiko, V.V., et al., “Epitaxial growthof GaAs on YSZ substrutes”, Abstr. 11-th Intern. Conf. Of Cryst. Growth. (The Hague, The Netherlands, 1995) 333 Google Scholar
Busynin, A.N., Buzynin, Yu.N., Osiko, V.V., Sov. Union Patent N1730872 (1992)Google Scholar
Aleksandrov, V.I., Osiko, V.V., Prokhorov, A.M. and Tatarintsev, V.M., “Synthesis and crystal growth of refractory materials by RF melting in a cold container”, in Current Topics in Materials Science, edited by , E. (North-Holland, Amsterdam, 1978), p.421 Google Scholar
Shabunov, V., Shengurov, V.N., Buzynin, A.N., et al., “Silicon heterostructures on fianite substrates:, Microelectronics 6, 204 (1996)Google Scholar
Soviet Union Patent N 1590027 (1991)Google Scholar
Sheftal, N.N. and Buzynin, A.N., “The epitaxy orientation of crystallites on amorphous substrute and effect of the stratches”, Vestnik Moscow Univ. 3, 102 (1972); Nat. Trans. Cent. The Yohn Crenan Library, 35w, 33rd St., Chicago IL 60616 USAGoogle Scholar
, S. D., Ramer, J. C., Malloy, K. J., MRS Bull. 22, 45 (1997).Google Scholar
Figure 0

Table I Some characteristics of YSZ and AIIIBV crystals.

Figure 1

Table II Impurity concentration in YSZ single crystals, YSZ-wafers and GaAs/YSZ films

Figure 2

Figure 1 SEM micrographs of GaAs films prepared using both conventional MOCVD (a) and capillary epitaxy MOCVD(b) at the initial stage of epitaxy on YSZ substrates (60 and 600s after procedure beginning, 20000x) and optical micrographs of NH4J flat crystals prepared by the graphoepitaxy technique on amorphous Al substrates without (c) and with(d) a surface active substance (100x).

Figure 3

Figure 2. Luminescence spectra of undoped GaN films on a YSZ substrate.