Hostname: page-component-586b7cd67f-g8jcs Total loading time: 0 Render date: 2024-12-01T01:32:36.980Z Has data issue: false hasContentIssue false

Growth of Epitaxial BaTiO3 Thin Films at 600°C by Metalorganic Chemical Vapor Deposition

Published online by Cambridge University Press:  15 February 2011

D.L. Kaiser
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
M.D. Vaudin
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
L.D. Rotter
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
Z.L. Wang
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
J.P. Cline
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
C.S. Hwang
Affiliation:
Materials Science and Engineering Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
R.B. Marinenko
Affiliation:
Chemical Science and Technology Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
J.G. Gillen
Affiliation:
Chemical Science and Technology Laboratory, National Institute of Standards and Technology, Gaithersburg, MD 20899
Get access

Abstract

Metalorganic chemical vapor deposition (MOCVD) was used to deposit epitaxial BaTiO3 thin films on (100) MgO substrates at 600°C. The metalorganic precursors employed in the deposition experiments were hydrated Ba(thd)2 (thd = C11H19O2) and titanium isopropoxide. The films were analyzed by means of transmittance spectroscopy, wavelength dispersive x-ray spectrometry, secondary ion mass spectrometry depth profiling, x-ray diffraction, high resolution transmission electron microscopy, selected area electron diffraction, nanoscale energy dispersive x-ray spectrometry and second harmonic generation measurements. There was no evidence for interdiffusion between the film and substrate. The x-ray and electron diffraction studies showed that the films were oriented with the a-axis normal to the substrate surface, whereas second harmonic generation measurements showed that the films had some c-axis character.

Type
Research Article
Copyright
Copyright © Materials Research Society 1995

Access options

Get access to the full version of this content by using one of the access options below. (Log in options will check for institutional or personal access. Content may require purchase if you do not have access.)

References

REFERENCES

1. Glass, A.M., Mater. Res. Bull. XIII (8), 16 (1988).Google Scholar
2. See e.g., Chapters 10 and 11 in Yeh, P., Introduction to Photorefractive Nonlinear Optics (Wiley, New York, 1993).Google Scholar
3. Armstrong, J.A., Bloemberger, B., Ducuing, J., and Persham, P.S., Phys. Rev. 127, 1918 (1962).Google Scholar
4. Nakazawa, H., Yamane, H., and Hirai, T., Jpn. J. Appl. Phys. 30, 2200 (1991).Google Scholar
5. Wills, L.A., Wessels, B.W., Richeson, D.S., and Marks, T.J., Appl. Phys. Lett. 60, 41 (1992).Google Scholar
6. Van Buskirk, P.C., Gardiner, R., Kirlin, P.S., and Nutt, S., J. Mater. Res. 7, 542 (1992).Google Scholar
7. Chern, C.S., Zhao, J., Luo, L., Lu, P., Li, Y.Q., Norris, P., Kear, B., Cosandey, F., Maggiore, B.J., Gallois, B., and Wilkens, B.J., Appl. Phys. Lett. 60, 1144 (1992).Google Scholar
8. Van Buskirk, P.C., Stauf, G.T., Gardiner, R., Kirlin, P.S., Bihari, B., and Kumar, J., in Ferroelectric Thin Films III, edited by Tuttle, B.A., Myers, E.R., Desu, S.B., and Larsen, P.K. (Mater. Res. Soc. Proc. 310, Pittsburgh, PA, 1993), pp. 119124.Google Scholar
9. Wolf, S. and Tauber, R.N., Silicon Processing for the VLSI Era, Vol. 1 (Lattice Press, Sunset Beach, CA, 1986), p. 57.Google Scholar
10. Kaiser, D.L., Vaudin, M.D., Gillen, G., Hwang, C.-S., Robins, L.H., and Rotter, L.D., J. Crystal Growth 137, 136 (1994).Google Scholar
11. Kaiser, D.L., Vaudin, M.D., Gillen, G., Hwang, C.-S., Robins, L.H., and Rotter, L.D., in Metal-Organic Chemical Vapor Deposition of Electronic Ceramics, edited by Desu, S.B., Beach, D.B., Wessels, B.W., and Gokoglu, S. (Mater. Res. Soc. Proc. 335, Pittsburgh, PA, 1994), pp. 4752.Google Scholar
12. Swanepoel, R., J. Phys. E: Sci. Instrum. 16, 1214 (1983).Google Scholar
13. Private Communication, Frank Wagner, Strem Chemicals, Inc.Google Scholar
14. Rushman, D.F., and Strivens, M.A., Faraday Soc. Trans. 42A, 231 (1946).Google Scholar
15. Reed-Hill, R.E., Physical Metallurgy Principles, Second Edition (D. Van Nostrand Co., New York, NY, 1973), pp. 157158.Google Scholar