Hostname: page-component-cd9895bd7-fscjk Total loading time: 0 Render date: 2024-12-25T14:18:03.522Z Has data issue: false hasContentIssue false

Rapid growth of a long-seed KDP crystal

Published online by Cambridge University Press:  19 February 2020

Duanyang Chen
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China Center of Materials Science and Optoelectronics Engineering, University of Chinese Academy of Sciences, Beijing100049, China
Bin Wang
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Hu Wang
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Xiangyu Zhu
Affiliation:
School of Aerospace Engineering, Tsinghua University, Beijing100084, China
Ziyuan Xu
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Yuanan Zhao
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Shenghao Wang
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Kaizao Ni
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Lili Zheng
Affiliation:
School of Aerospace Engineering, Tsinghua University, Beijing100084, China
Hui Zhang
Affiliation:
Department of Engineering Physics, Tsinghua University, Beijing100084, China
Hongji Qi*
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
Jianda Shao*
Affiliation:
Key Laboratory of Materials for High Power Laser, Shanghai Institute of Optics and Fine Mechanics, Chinese Academy of Sciences, Shanghai201800, China
*
Correspondence to:  H. Qi and J. Shao, No. 390 Qinghe Road, Jiading District, Shanghai 201800, China. Email: [email protected] (H. Qi); [email protected] (J. Shao)
Correspondence to:  H. Qi and J. Shao, No. 390 Qinghe Road, Jiading District, Shanghai 201800, China. Email: [email protected] (H. Qi); [email protected] (J. Shao)

Abstract

To reduce the seed length while maintaining the advantages of the cuboid KDP-type crystal, a long-seed KDP crystal with size $471~\text{mm}\times 480~\text{mm}\times 400~\text{mm}$ is rapidly grown. With almost the same high cutting efficiency to obtain third harmonic generation oriented samples, this long-seed KDP-type crystal can be grown with a shorter seed than that of the cuboid KDP-type crystal. The full width at half maximum of the high-resolution X-ray diffraction of the (200) crystalline face is 28.8 arc seconds, indicating that the long-seed KDP crystal has good crystalline quality. In the wavelength range of 377–1022 nm, the transmittance of the long-seed KDP crystal is higher than 90%. The fluence for the 50% probability of laser-induced damage (LID) is $18.5~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm). Several test points survive when the laser fluence exceeds $30~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm), indicating the good LID performance of the long-seed KDP crystal. At present, the growth of a long-seed DKDP crystal is under way.

Type
Research Article
Creative Commons
Creative Common License - CCCreative Common License - BY
This is an Open Access article, distributed under the terms of the Creative Commons Attribution licence (http://creativecommons.org/licenses/by/4.0/), which permits unrestricted re-use, distribution, and reproduction in any medium, provided the original work is properly cited.
Copyright
© The Author(s) 2020

1 Introduction

The high-power lasers used in the inertial confinement fusion (ICF) system worldwide need large KDP-type crystals as nonlinear crystals on account of their exceptional properties[Reference De Yoreo, Burnham and Whitman1Reference Cai, Lin, Li, Lu, Hu and Zheng6]. The major limitation to growing such large KDP-type crystals by the traditional method is the slow growth rate, leading to a growth cycle of 1–2 years[Reference Wang, Li, Wang, Wang, Wang, Ding, Li, Shen, Liu and Huang7Reference Li, Yu, Wang, Ding, Xu, Gu, Wang and Huang11]. Fortunately, the ‘point-seed’ rapid growth method was developed in the 1980s[Reference Zaitseva and Carman12, Reference Wang, Shen, Lan, Huang, Cui, Kang, Niu, Wang, Wang and Boughton13]. For the KDP-type crystals produced by the ‘point-seed’ rapid growth method, all prismatic faces and pyramidal faces develop under high supersaturated solutions[Reference Land, Martin, Potapenko, Palmore and De Yoreo14Reference Pommies, Damiani, Bertussi, Capoulade, Piombini, Natoli and Mathis17]. In addition, a pyramid–prism (PY–PR) boundary is generated when different kinds of crystallographic faces are sewn together[Reference Chen, Wang, Wang, Bai, Xu, Li, Qi and Shao18Reference Yan, Torres, Runkel, Woods, Hutcheon, Zaitseva and De Yoreo21]. By the orthogonal polarization interferometry technology, $\unicode[STIX]{x0394}(n_{e}{-}n_{o})$ maps containing the PY–PR boundary were easily obtained, and the distortion near the PY–PR boundary was reported to be detrimental to efficient frequency tripling and phase matching[Reference Li, Zheng, Qi, Yin, Tang, Li, Xu, Lei, Lin, Zhang, Lu, Ma, He and Yao22, Reference Auerbach, Wegner, Couture, Eimerl, Hibbard, Milam and Hackel23]. More recently, a cuboid DKDP crystal was rapidly grown[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. Without a pyramidal sector, the cuboid DKDP crystal had high cutting efficiency to obtain third harmonic generation (THG)-oriented samples for ICF. However, in practice, it is not always easy to get a long seed to grow a large cuboid KDP-type crystal. Therefore, it is of practical significance to reduce the length of the seed while maintaining the advantages of the cuboid KDP-type crystal.

In this study, a long-seed KDP crystal was rapidly grown. With almost the same high cutting efficiency to obtain THG-oriented samples, this long-seed KDP-type crystal can grow from a seed that is shorter than that of the cuboid KDP-type crystal. Then the crystalline quality, transmittance performance, laser-induced damage (LID) property and LID morphology of the long-seed KDP crystal were investigated.

2 Experimental setup

2.1 Crystal growth

The long-seed KDP crystal was rapidly grown in a self-developed 2000 L growth apparatus configured as an efficient continuous filtration system (CFS)[Reference Xie, Qi, Wang, Wang, Chen and Shao25, Reference Hu, Wang, Chang, Xie, Zhao, Qi and Shao26]. A long KDP seed with size $20~\text{mm}\times 20~\text{mm}\times 260~\text{mm}$ was fixed on a crystal carrier, and the length direction of the seed crystal was the [001] crystallography direction. During crystal growth, the supersaturation of the solution was approximately 5%, and the crystal carrier was rotated in alternative cycles[Reference Robey and Maynes27, Reference Robey28]. After 70 days, a long-seed KDP crystal with dimensions $471~\text{mm}\times 480~\text{mm}\times 400~\text{mm}$ and weight 254 kg was grown, as shown in Figure 1. It is worth mentioning that there is no visible defect in the long-seed KDP crystal. In addition, the growth of a long-seed DKDP crystal is currently under way.

Figure 1. Long-seed KDP crystal with size $471~\text{mm}\times 480~\text{mm}\times 400~\text{mm}$.

2.2 Characterization techniques

To evaluate the properties of the long-seed KDP crystal, the high-resolution X-ray diffraction (HRXRD) of an X-cut sample from this crystal was carried out[Reference Sharma, Verma, Singh and Bartwal29]. The transmission spectrum of a THG-oriented sample cut from the long-seed KDP crystal was tested using a Lambda 1050 spectrometer[Reference Chen, Wang, Wang, Bai, Xu, Li, Qi and Shao18]. The LID threshold (LIDT) at 355 nm of the THG-oriented sample was investigated under a Nd:YAG laser[Reference Peng, Zhao, Wang, Hu, Yang and Shao30]. The LID scattering image of the THG-oriented sample was captured by an online microscope system mounted on the laser damage facility, and the morphology of the LID bulk was observed by an offline polarization microscope[Reference Wu, Zhao, Wang, Peng, Yang, Shan and Shao31].

3 Results and discussion

3.1 Advantages of cut THG-oriented samples

The THG-oriented samples cut from the cuboid KDP-type crystal and the long-seed KDP-type crystal are shown in Figure 2. As in our previous work, the number $N$ of THG-oriented samples cut from the cuboid KDP-type crystal follows the formulas below[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]:

(1)$$\begin{eqnarray}\displaystyle (T\sin \unicode[STIX]{x1D6FC}+V)\times 2+s=L, & & \displaystyle\end{eqnarray}$$
(2)$$\begin{eqnarray}\displaystyle W\sin \unicode[STIX]{x1D6FC}+T\cos \unicode[STIX]{x1D6FC}+IN/2=H, & & \displaystyle\end{eqnarray}$$

where $L$, $W$ and $T$ are the length, width and thickness of the largest THG-oriented sample that can be cut from the cuboid KDP-type crystal. The height of the cuboid KDP-type crystal is $H$, the width of the seed is $s$ and the phase-matching angle of the THG-oriented sample is $\unicode[STIX]{x1D6FC}$. The parameters $V$ and $I$ represent the width of the projection of the sample on the horizontal plane and the spacing of the adjacent two samples in the direction of height, respectively.

For simplicity, $\unicode[STIX]{x1D6FC}$ and $s$ are approximately equal to $60^{\circ }$ and 15 mm, respectively; $V$ and $I$ are equal to $W\cos \unicode[STIX]{x1D6FC}$ and $T/\cos \unicode[STIX]{x1D6FC}$, respectively. The above two formulas can be simplified as follows:

(3)$$\begin{eqnarray}\displaystyle (0.886T+0.5W)\times 2+15=L, & & \displaystyle\end{eqnarray}$$
(4)$$\begin{eqnarray}\displaystyle 0.886W+0.5T+NT=H. & & \displaystyle\end{eqnarray}$$

Therefore, to get 10 ($N=10$) THG-oriented samples with size $460~\text{mm}\times 430~\text{mm}\times 10~\text{mm}$ ($W=430$, $T=10$, $L=(0.886T+0.5W)\times 2+15\approx 460$), the cuboid KDP-type crystal should grow to size of $460~\text{mm}\times 460~\text{mm}\times 486~\text{mm}$ ($H=0.886W+0.5T+NT=486$), and the length of the seed should also be 486 mm.

For the long-seed KDP-type crystal, the growth rate in the horizontal and vertical directions is approximately 3:2, according to the crystal grown in this study. Equations (1)–(4) are also applicable to the long-seed KDP-type crystal, with only minor corrections in height. Equation (2) can be approximately changed to

(5)$$\begin{eqnarray}\displaystyle W\sin \unicode[STIX]{x1D6FC}+T\cos \unicode[STIX]{x1D6FC}+IN/2+T=H. & & \displaystyle\end{eqnarray}$$

Therefore, to get 10 ($N=10$) THG-oriented samples with size $460~\text{mm}\times 430~\text{mm}\times 10~\text{mm}$, the long-seed KDP-type crystal should grow to size $460~\text{mm}\times 460~\text{mm}\times 496~\text{mm}$ ($H=0.886W+0.5T+NT+T=496$). Since the prismatic face grew by about 222 mm, the crystal grew by approximately 148 mm in the length direction. So a seed with length 348 mm is sufficient. As mentioned above, the length of the seed is 486 mm for the cuboid KDP-type crystal. For the long-seed KDP-type crystal, the seed crystal can be shortened by 138 mm in this case.

Figure 2. THG-oriented samples cut from the cuboid KDP-type crystal (left) and the long-seed KDP-type crystal (right).

3.2 Crystalline quality of the long-seed KDP crystal

The HRXRD pattern of the (200) crystalline face cut from the long-seed KDP crystal is shown in Figure 3. The full width at half maximum (FWHM) of the HRXRD is 28.8 arc seconds, indicating that the long-seed KDP crystal has good crystalline quality. More details about the testing can be found in other articles[Reference Chen, Wang, Wang, Bai, Xu, Li, Qi and Shao18, Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. As defined by the plane wave dynamic theory of X-ray diffraction, a smaller value of FWHM indicates better crystallinity[Reference Ramteke, Anis, Baig, Algarni and Muley32, Reference Anis, Baig, Pandian, Ramasamy, AlFaify, Ganesh, Muley and Ghramh33]. For the cuboid DKDP crystal, the FWHM of the HRXRD is also 28.8 arc seconds, indicating that there is no essential difference in crystalline quality between the cuboid KDP-type crystal and the long-seed KDP-type crystal[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24].

Figure 3. HRXRD pattern of the long-seed KDP crystal.

3.3 Transmittance of the long-seed KDP crystal

The transmission spectrum of a THG-oriented sample of the long-seed KDP crystal is shown in Figure 4. The vibration near 860 nm was caused by switching the detectors of the spectrometer at this wavelength. In the wavelength range of 377–1022 nm, the transmittance is higher than 90%, which is almost the same as that of the cuboid DKDP crystal. The transmittance at 355 nm is 82.9%, a little higher than that of the cuboid DKDP crystal[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. The various factors responsible for the origin and influence of optical transmittance can be found from peer-reviewed literature[Reference Azhar, Anis, Rabbani, Shirsat, Baig, Hussaini, AlFaify and Khan34Reference AlFaify, Shkir, Ganesh, Anis and Yahia36].

Figure 4. Transmittance of the long-seed KDP crystal.

3.4 Laser-induced damage property

The LID property at 355 nm of the THG-oriented sample cut from the long-seed KDP crystal is shown in Figure 5. The effective area of the laser spot is $0.26~\text{mm}^{2}$. The fluence for the 50% probability of LID is $18.5~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm), 38% higher than that of the cuboid DKDP crystal[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. Several test points survive when the laser fluence exceeds $30~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm), indicating the good LID property of the long-seed KDP crystal.

Figure 5. LIDT of the long-seed KDP crystal.

Table 1. Fitting of different kinds of defects.

A model is used to quantify the LID property of the long-seed KDP crystal[Reference Natoli, Gallais, Akhouayri and Amra37, Reference Krol, Gallais, Grezes-Besset, Natoli and Commandre38]. In Figure 5, three types of defects are fitted. The fitted LIDT and density of different kinds of defects are shown in Table 1. The density is $0.063~\text{mm}^{-3}$ for the defect that has the lowest LIDT, indicating that defects that can easily induce damage under 355 nm in the long-seed KDP crystal are rare. Some extrinsic factors such as incident photon energy, pulse width and polarization mode and intrinsic factors such as thermal expansion coefficient, electron avalanche breakdown and nonlinear absorption effects play decisive roles in laser damage properties of crystalline materials. Detailed explanations are given in Refs. [Reference Ramteke, Kalainathan, Anis, Muley, Baig and Algarni39Reference Azhar, Hussaini, Shirsat, Rabbani, Shkir, Alfaify, Ghramh, Baig and Anis41].

3.5 Laser-induced damage morphology

Illuminated by a 532 nm probe laser, the LID scattering image of the THG-oriented sample is recorded by an online microscope system mounted on the laser damage facility. The microscope is placed orthogonally to the propagation direction of the 355 nm laser. Once the damage happens, the microscope immediately captures the LID scattering image. An LID scattering image at 30 J/cm2 (3 ns, 355 nm), is shown in Figure 6, with length about 10 mm, which is also the thickness of the sample. Even at such a high fluence, only three damage points appear within 10 mm, indicating that the long-seed KDP crystal has good damage resistance. Although it looks like six scattering points in the figure, there are actually only three LID points. Because of birefringence, the scattered light of each LID point is split into two beams (namely the o light and e light), forming two scattering points in the microscope.

Figure 6. LID scattering image at $30~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm).

The morphology of the damage points in Figure 6 is observed by an offline polarization microscope. The morphology of damage points in Figure 7 from left to right shows exactly the same points as in Figure 6. In Figure 7, all the damage points consist of a core, a distortion zone around the core and cracks extending from the core[Reference Hu, Zhao, Li and Xiao42, Reference Carr, Feit, Johnson and Rubenchik43]. Because the sample did not rotate when testing the morphology of the three points, all the cracks extend in only two directions, which should be the directions of the crystalline axes[Reference Burnham, Runkel, Feit, Rubenchik, Floyd, Land, Siekhaus and Hawley-Fedder44Reference Yoshida, Jitsuno, Fujita, Nakatsuka, Yoshimura, Sasaki and Yoshida46]. An approach to evaluate damage performance provides statistics on damage pinpoint density, size and morphology as a function of fluence, wavelength and pulse duration and relates that to the resulting beam obscuration[Reference DeMange, Carr, Radousky and Demos47]. The power limitation was found to play a vital role in the use of rapidly grown KDP-type crystals in the ICF system.

Figure 7. Morphology of the LID bulks in Figure 6.

4 Conclusions

Despite being the subject of study for more than 30 years, rapidly grown KDP-type crystals are still grown from a ‘point seed’. In this study, a long-seed KDP crystal with size $471~\text{mm}\times 480~\text{mm}\times 400~\text{mm}$ was rapidly grown. With almost the same high cutting efficiency to obtain THG-oriented samples, this long-seed KDP-type crystal can grow from a seed that is shorter than that of the cuboid KDP-type crystal proposed in the recently published literature[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. For example, to get 10 THG-oriented samples with size $460~\text{mm}\times 430~\text{mm}\times 10~\text{mm}$, the size of the seed should be at least 486 mm for the cuboid KDP-type crystal, while it is just 348 mm for the long-seed KDP-type crystal. Therefore, it is of practical significance since it is not always easy to get a long seed to grow a large cuboid KDP-type crystal. The long-seed KDP crystal also exhibits good crystalline quality since the FWHM of HRXRD is the same as that of the cuboid DKDP crystal[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. As to the transmission and the LID performance, the long-seed KDP crystal is even better than the cuboid DKDP crystal[Reference Chen, Wang, Wang, Zheng, Zhang, Qi and Shao24]. Furthermore, new seeds with much longer size in the [001] crystallography direction than the original seed can be taken from the pyramidal portion down through the prismatic portion. In addition, because the carrier has a height greater than that of the long seed, there is no need to replace the carrier for a different seed with that of different height. For the cuboid KDP-type crystal, once the height of the carrier is set, the length of the seed must be equal to the height of the carrier. Therefore, the long-seed KDP-type crystal is more promising than the cuboid KDP-type crystal in engineering application.

Acknowledgement

This work was supported by the National Natural Science Foundation of China (No. 11535010).

References

De Yoreo, J. J.Burnham, A. K. and Whitman, P. K.Int. Mater. Rev. 47, 113 (2002).CrossRefGoogle Scholar
Huang, P.Ding, J.Wang, D.Liu, H.Xu, L.Li, X.Wang, B.Liu, G. and Wang, S.CrystEngComm 21, 1329 (2019).CrossRefGoogle Scholar
Piquard, J.Zaccaro, J.Pintault, B.Maunier, C. and Ibanez, A.CrystEngComm 21, 372 (2019).CrossRefGoogle Scholar
Huang, P.Wang, S.Wang, D.Liu, H.Liu, G. and Xu, L.CrystEngComm 20, 3171 (2018).CrossRefGoogle Scholar
Sun, C. and Xue, D.CrystEngComm 15, 10445 (2013).CrossRefGoogle Scholar
Cai, X.Lin, X.Li, G.Lu, J.Hu, Z. and Zheng, G.High Power Laser Sci 7, e46 (2019).CrossRefGoogle Scholar
Wang, D.Li, T.Wang, S.Wang, J.Wang, Z.Ding, J.Li, W.Shen, C.Liu, G. and Huang, P.CrystEngComm 18, 9292 (2016).CrossRefGoogle Scholar
Khan, I.Kalainathan, S.Baig, M. I.Shkir, M.Alfaify, S.Ghramh, H. A. and Anis, M.Materials Science-Poland 36, 662 (2018).CrossRefGoogle Scholar
Anis, M.Muley, G. G.Baig, M. I.Rabbani, G.Ghramhans, H. A. and Ramteke, S. P.Optik 178, 752 (2019).CrossRefGoogle Scholar
Baig, M. I.Anis, M. and Muley, G. G.Opt. Mater. 72, 1 (2017).CrossRefGoogle Scholar
Li, W.Yu, G.Wang, S.Ding, J.Xu, X.Gu, Q.Wang, D. and Huang, P.RSC Adv. 7, 17531 (2017).CrossRefGoogle Scholar
Zaitseva, N. and Carman, L.Prog. Cryst. Growth Charact. Mater. 43, 1 (2001).CrossRefGoogle Scholar
Wang, D.Shen, C.Lan, J.Huang, P.Cui, Z.Kang, T.Niu, Y.Wang, S.Wang, J. and Boughton, R. I.J. Alloys Compd. 790, 212 (2019).CrossRefGoogle Scholar
Land, T. A.Martin, T. L.Potapenko, S.Palmore, G. T. and De Yoreo, J. J.Nature 399, 442 (1999).CrossRefGoogle Scholar
Tu, H.Zhao, Y.Yue, Y.Fan, F. and Hu, Z.CrystEngComm 17, 6669 (2015).CrossRefGoogle Scholar
Hawley-Fedder, R.Geraghty, P.Locke, S.McBurney, M.Runkel, M.Suratwala, T.Thompson, S.Wegner, P. and Whitman, P.Proc. SPIE 5341, 121 (2004).CrossRefGoogle Scholar
Pommies, M.Damiani, D.Bertussi, B.Capoulade, J.Piombini, H.Natoli, J. Y. and Mathis, H.Opt. Commun. 267, 154 (2006).CrossRefGoogle Scholar
Chen, D.Wang, B.Wang, H.Bai, Y.Xu, N.Li, B.Qi, H. and Shao, J.CrystEngComm 21, 1482 (2019).CrossRefGoogle Scholar
Negres, R. A.Zaitseva, N. P.DeMange, P. and Demos, S. G.Proc. SPIE 6403, 64031S (2006).CrossRefGoogle Scholar
Surmin, A.Guillet, F.Lambert, S.Damiani, D. and Pommiès, M.Proc. SPIE 5991, 59911W (2005).CrossRefGoogle Scholar
Yan, M.Torres, R. A.Runkel, M. J.Woods, B. W.Hutcheon, I. D.Zaitseva, N. P. and De Yoreo, J. J.Proc. SPIE 2966, 11 (1996).CrossRefGoogle Scholar
Li, G.Zheng, G.Qi, Y.Yin, P.Tang, E.Li, F.Xu, J.Lei, T.Lin, X.Zhang, M.Lu, J.Ma, J.He, Y. and Yao, Y.High Power Laser Sci. 2, e2 (2014).CrossRefGoogle Scholar
Auerbach, J. M.Wegner, P. J.Couture, S. A.Eimerl, D.Hibbard, R. L.Milam, D. and Hackel, L. A.Appl. Opt. 40, 1404 (2001).CrossRefGoogle Scholar
Chen, D.Wang, B.Wang, H.Zheng, L.Zhang, H.Qi, H. and Shao, J.Cryst. Growth Des. 19, 2746 (2019).CrossRefGoogle Scholar
Xie, X.Qi, H.Wang, B.Wang, H.Chen, D. and Shao, J.J. Cryst. Growth 487, 45 (2018).CrossRefGoogle Scholar
Hu, G.Wang, Y.Chang, J.Xie, X.Zhao, Y.Qi, H. and Shao, J.High Power Laser Sci. 3, e13 (2015).CrossRefGoogle Scholar
Robey, H. F. and Maynes, D.J. Cryst. Growth 222, 263 (2001).CrossRefGoogle Scholar
Robey, H. F.J. Cryst. Growth 259, 388 (2003).CrossRefGoogle Scholar
Sharma, S. K.Verma, S.Singh, Y. and Bartwal, K. S.CrystEngComm 15, 9955 (2013).CrossRefGoogle Scholar
Peng, X.Zhao, Y.Wang, Y.Hu, G.Yang, L. and Shao, J.Chin. Opt. Lett. 16, 051601 (2018).CrossRefGoogle Scholar
Wu, J.Zhao, Y.Wang, L.Peng, X.Yang, L.Shan, C. and Shao, J.Chin. J. Lasers 46, 0501003 (2019).Google Scholar
Ramteke, S. P.Anis, M.Baig, M. I.Algarni, H. and Muley, G. G.Optik 197, 163219 (2019).CrossRefGoogle Scholar
Anis, M.Baig, M. I.Pandian, M. S.Ramasamy, P.AlFaify, S.Ganesh, V.Muley, G. G. and Ghramh, H. A.Cryst. Res. Technol. 53, 1700165 (2018).CrossRefGoogle Scholar
Azhar, S. M.Anis, M.Rabbani, G.Shirsat, M. D.Baig, M. I.Hussaini, S. S.AlFaify, S. and Khan, M. A.Optik 185, 1247 (2019).CrossRefGoogle Scholar
Anis, M.Baig, M. I.Muley, G. G.Rabbani, G.Shirsat, M. D.Shkir, M. and Ghramh, H. A.Mater. Lett. 233, 238 (2018).CrossRefGoogle Scholar
AlFaify, S.Shkir, M.Ganesh, V.Anis, M. and Yahia, I. S.Appl. Phys. B 124, 196 (2018).CrossRefGoogle Scholar
Natoli, J. Y.Gallais, L.Akhouayri, H. and Amra, C.Appl. Opt. 41, 3156 (2002).CrossRefGoogle Scholar
Krol, H.Gallais, L.Grezes-Besset, C.Natoli, J. Y. and Commandre, M.Opt. Commun. 256, 184 (2005).CrossRefGoogle Scholar
Ramteke, S. P.Kalainathan, S.Anis, M.Muley, G. G.Baig, M. I. and Algarni, H.Optik 201, 163509 (2020).CrossRefGoogle Scholar
Ramteke, S. P.Baig, M. I.Shkir, M.Kalainathan, S.Shirsat, M. D.Muley, G. G. and Anis, M.Opt. Laser Technol. 104, 83 (2018).CrossRefGoogle Scholar
Azhar, S. M.Hussaini, S. S.Shirsat, M. D.Rabbani, G.Shkir, M.Alfaify, S.Ghramh, H. A.Baig, M. I. and Anis, M.Mater. Res. Innov. 23, 123 (2019).CrossRefGoogle Scholar
Hu, G.Zhao, Y.Li, D. and Xiao, Q.Chin. Phys. Lett. 29, 037801 (2012).CrossRefGoogle Scholar
Carr, C. W.Feit, M. D.Johnson, M. A. and Rubenchik, A. M.Appl. Phys. Lett. 89, 131901 (2006).CrossRefGoogle Scholar
Burnham, A. K.Runkel, M.Feit, M. D.Rubenchik, A. M.Floyd, R. L.Land, T. A.Siekhaus, W. J. and Hawley-Fedder, R. A.Appl. Opt. 42, 5483 (2003).CrossRefGoogle Scholar
Jiang, H.McNary, J.Tom, H. W. K.Yan, M.Radousky, H. B. and Demos, S. G.Appl. Phys. Lett. 81, 3149 (2002).CrossRefGoogle Scholar
Yoshida, H.Jitsuno, T.Fujita, H.Nakatsuka, M.Yoshimura, M.Sasaki, T. and Yoshida, K.Appl. Phys. B 70, 195 (2000).CrossRefGoogle Scholar
DeMange, P.Carr, C. W.Radousky, H. B. and Demos, S. G.Proc. SPIE 5337, 47 (2004).CrossRefGoogle Scholar
Figure 0

Figure 1. Long-seed KDP crystal with size $471~\text{mm}\times 480~\text{mm}\times 400~\text{mm}$.

Figure 1

Figure 2. THG-oriented samples cut from the cuboid KDP-type crystal (left) and the long-seed KDP-type crystal (right).

Figure 2

Figure 3. HRXRD pattern of the long-seed KDP crystal.

Figure 3

Figure 4. Transmittance of the long-seed KDP crystal.

Figure 4

Figure 5. LIDT of the long-seed KDP crystal.

Figure 5

Table 1. Fitting of different kinds of defects.

Figure 6

Figure 6. LID scattering image at $30~\text{J}/\text{cm}^{2}$ (3 ns, 355 nm).

Figure 7

Figure 7. Morphology of the LID bulks in Figure 6.